1.
Mix glue and hardener in 20/1 ratio.
After
that,
the
approximate life span of 1-2 hours.
2.
Apply a thin coat of the adhesive with
a brush to both surfaces. On the boat skin
an overlap of 2 mm should be included.
3.
Let it cure for 30 min. It needs to be
dry!
4.
Repeat the brushing.
5.
Let it cure again for 10 min (The
adhesive must be completely dry, test by
touching if necessary).
62
Anfibio Packrafting, Schellin & Kreinacker GbR, Körnerplatz 3d, 04107 Leipzig, Tel.:+49(0) 341/39281264, www.anfibio.com
Repairs at home:
Larger tears should be repaired with the original
material. For bonding we recommend the special PU glue
"Helaplast".
The gluing performs best in a dry, well-ventilated
room at a temperature of about 15-25 °C.
mixture
has
an
6.
Position the patch on the damaged
area. The parts will not stick yet so you
can easily move it to the correct position.
7.
Apply heat to the parts by fan with at
least 70°C, which reactivates the glue.
The parts will stick together strongly.
Remember to press firmly.
8.
After that the parts are fixed
together. The adhesive connection has
already reached 80% of its final
strength. Allow a further 36 hours for
the hardening to finish.